How can one accomplish a subcritical anneal without an oven or salts? Should I heat to 1300F and then soak in vermiculite until cool?
Here are the thermal cycles I do to prep for the anneal (thanks to everyone in this forum for helping me come up with this or posting so I can try out your ideas!):
1084
1. Normalize: 1600 F and air cool
2. Thermal Cycling: once to 1500-1475 F with air cool, once 1450-1475 F with oil quench, 3 cycles from 1275 to black cooling in air
W2
1. Normalize: 1600 F and air cool
2. Thermal Cycling with air cooling to black heat between cycles:
a. once to 1475 F
b. once to 1450 F
c. once to 1425 F
Perhaps with the 1084, the 3 cycles to 1275 F act as the anneal? Any advice or observations are welcome.
Apprentice Smith
www.feathercapforge.com
#2
Posted 16 May 2012 - 06:53 PM
Apprentice Smith
#3
Posted 16 May 2012 - 07:59 PM
Wood ash or lime will also work.
You might want to check out Kevin's website for additional information.
Kevin Cashen bladesmithing info
Brion
Anvil Top Custom Knives
ABS Mastersmith
#4
Posted 17 May 2012 - 05:49 AM
With rampable kilns soaking at 1375F before cooling at a rate of less than 50F per hour is the most thorough way to spheroidized. Without such a kiln heating to 1275F, but not more than 1300F, (dull red but keep the magnet sticking) should ball up your extra carbides. All of the real work is done from 900F to 1275F so there is no great need for insulating on the cool. Heck all the of the real work in traditional annealing is done in the same range so once the steel is lower than 900F there is no reason for a slow cool there either. In fact some industrial processes rapidly cool to the correct range and then once the desired effects are obtained the steel can be quenched to room temp and immediately worked, but that requires exact temperature control.
#6
Posted 17 May 2012 - 09:43 AM
Cheyenne Walker, on 17 May 2012 - 10:02 AM, said:
O-1 almost necessitates spheroidizing (aka sub critical anneal), in fact if I were going to machine it I would do nothing less than a full industrial spheroidizing.
#7
Posted 17 May 2012 - 09:51 AM
BrionTomberlin, on 16 May 2012 - 09:59 PM, said:
Wood ash or lime will also work.
You might want to check out Kevin's website for additional information.
Kevin Cashen bladesmithing info
Brion
Brion,
Do you do the process above on both 1084 and W2? I was thinking that the thermal cycling had to be in the higher ranges for the W2....but I'm not sure why.
It's good to hear of someone using vermiculite from a subcritical anneal--I thought vermiculite was used for the slow cool only from higher temperatures (Again, I'm not sure why I thought that either).
Apprentice Smith
www.feathercapforge.com
#8
Posted 17 May 2012 - 10:46 AM
Kevin R. Cashen, on 17 May 2012 - 07:49 AM, said:
With rampable kilns soaking at 1375F before cooling at a rate of less than 50F per hour is the most thorough way to spheroidized. Without such a kiln heating to 1275F, but not more than 1300F, (dull red but keep the magnet sticking) should ball up your extra carbides. All of the real work is done from 900F to 1275F so there is no great need for insulating on the cool. Heck all the of the real work in traditional annealing is done in the same range so once the steel is lower than 900F there is no reason for a slow cool there either. In fact some industrial processes rapidly cool to the correct range and then once the desired effects are obtained the steel can be quenched to room temp and immediately worked, but that requires exact temperature control.
Kevin--thanks for jumping in. I was pretty comfortable with the 1084 heat cycling since you and several others helped me work it out in an earlier thread. The W2 cycling I lifted from the hamon thread, but the subcritical anneal step I couldn't do because I don't have an oven.
So, are you saying that a good substitute for the oven soak and slow oven cool to 900 (50 F/hour) anneal is to heat to 1275 F and then air cool? Should I do three cycles, like with the 1084?
Apprentice Smith
www.feathercapforge.com
#9
Posted 17 May 2012 - 04:33 PM
Steve Morley, on 17 May 2012 - 12:46 PM, said:
So, are you saying that a good substitute for the oven soak and slow oven cool to 900 (50 F/hour) anneal is to heat to 1275 F and then air cool? Should I do three cycles, like with the 1084?
Multiple cycles can work if you are not able to hold for any ammount of time.
#10
Posted 26 May 2012 - 10:27 PM
Steve Morley, on 15 May 2012 - 07:07 PM, said:
1. Normalize: 1600 F and air cool
2. Thermal Cycling: once to 1500-1475 F with air cool, once 1450-1475 F with oil quench, 3 cycles from 1275 to black cooling in air.
Steve,
On the 1084 only...
The 1600F normalize made all grains the same size... bigger than ideal but equal in size. Stepping down the temperature for the next normalizing cycle kept the grains equal in size and made them smaller. Quenching after the next step down in temperature (third normalizing cycle) had the grains equal in size and smaller yet.. AND added a large amount of strain to all the crystals. 3 cycles at 1275 is a "jack shaft" spherodize anneal.
If you had skipped the quench after the third normalizing cycle you would have ended with grains small enough to advantage a knife blade and a piece of steel that was soft enough to grind, file, drill, and sand easily.
Annealing by cooling from above critical at a very slow rate will always cause grains to be large. Large grains are not the end of the world for a knife, but they don't have to be that way and it takes less time to make grains small and have steel (of eutectic carbon level and less) soft enough to work by normalizing three times, than to do a slow-cool anneal... (what do you call that kind of annneal, Kevin?)
Mike
#11
Posted 27 May 2012 - 06:14 AM
Mike Krall, on 27 May 2012 - 12:27 AM, said:
Mike
The actual technical term (and that recognized in industry) is "lamellar annealing", in simple carbon steels because it produces lamellar structures (pearlite). It does not necessarily have to produce coarse grain but it does have to produce grain size equal to that induced by the higher austenitizing temperature (how high that is is a matter of choice). So long as the grain coarsening temperature is not exceeded grain growth is solely a matter of temp and not time. What a lamellar will unavoidably do is create coarse carbide, which can be worse than grain size, depending how it is arranged and whether you can break it up again. Hypereutectoid steels will make large lamellar sheets and carbide networks when cooled slow from above critical. Spheroidizing tends to isolate the carbide into fine spheroids and obviously is well below anything that could even effect grain size.
#12
Posted 27 May 2012 - 11:37 AM
Kevin R. Cashen, on 27 May 2012 - 07:14 AM, said:
Thank you, Kevin...