Posted 25 September 2011 - 06:55 AM

I had the fun opportunity a couple weeks ago to forge weld for the first time at a friend's shop. Forged 2 San Mai blanks of his stock, L6 and 1080. Definitely some learning to be done on keeping my core going the right way and had some questions for you more experienced guys. Primarily, how much forging to shape do you try for? Also, once you accomplish the weld, how much are you trying to draw it out? I'm curious about these things because it seems they would have a significant effect on how it looks when you grind it and get that contrasting line. Is it similar in some ways to the mosaic damascus patterns where it's mostly stock removal after welding so as not to mess up the pattern? Hope that all makes sense and thanks for any tips.

Jeremy
Jeremy Lindley, Apprentice Smith
0

#2 User is offline   Lin Rhea 

  • Advanced Forum Member
  • PipPipPipPip
  • View gallery
  • Group: Members
  • Posts: 449
  • Joined: 04-February 10
  • LocationPrattsville, Arkansas
  • ABS Rating:Master Smith

Posted 25 September 2011 - 11:14 AM

Jeremy,
As the maker you have to be able to develope a vision of the intended blade and that includes the pattern and size. Once you have it welded, you are free to draw it out as you like, but here is the thing that will make it look right. You mentioned it already. Forge it evenly. Try to keep the pattern centered up in the blade. You will get a feel for it, but sometimes you may have to let it cool off during the forging process and grind off the scale and check it by dipping it in acid to actually see the pattern. If you have'nt gone too far with your forging, there might be opportunity to make corrections if need be.

Forging evenly. How do you do that? Besides the obvious, you should take into consideration that while you are hammering one side of the blade, the other is against the anvil and cooling faster. I try to hammer one side, then go back into the forge and then hammer the other. I try to keep the heat within a range, not allowing the blade to get close to being too cold. So, even heating, similar hammering techniques and patterns of progression along the blade as they relate to each side, is important.
Lin Rhea, ABS Mastersmith
Email me
0

#3 User is online   Brian Thie 

  • Advanced Forum Member
  • PipPipPipPip
  • View gallery
  • Group: Members
  • Posts: 168
  • Joined: 10-March 10
  • LocationBurlington, Iowa
  • ABS Rating:Journeyman Smith

Posted 25 September 2011 - 08:16 PM

Jeremy

Lin gave some great advise and as he said, you have to develop a vision of the finished piece. If you draw what you would like your finished blade to look like (especially where the transition line is where the 2 materials meet), it will help you answer the questions on how much forging you need to do.

The more you forge in the bevels and distal taper, the closer the transition (line where the 2 materials meet) will be to the edge.

Posted Image

The above diagram illustrates this. Each diagram has the 3 pieces and the darker lines represent the bevels of the blade converging at the cutting edge (everything on the outside of the darker lines represents what will be ground off). The image on the left would be a stock removal and the right would be the bevels forged very close to shape. You can see from this how you have control of the outcome by forging. Similarly, you should also be able to get a feel for how the thickness of each material can have an effect on the outcome.

Brian
Brian Thie
Journeyman Smith
www.mepotelco.net/web/tknives
0

#4 User is offline   Jeremy Lindley 

  • Advanced Forum Member
  • PipPipPipPip
  • Group: Members
  • Posts: 107
  • Joined: 17-June 11
  • LocationSouthwest Idaho
  • ABS Rating:Apprentice Smith

Posted 26 September 2011 - 06:16 AM

Thanks very much for the responses. For some reason I hadn't taken into account as much the forged bevels and how that would change the depth of the transition line-the drawings were very helpful. I guess the good thing is I have a few decent sized bars to work on and see how doing some different approaches on each changes the outcome. Then next time I have a better idea of where I want to go with it as well as paying closer attention to even forging on both sides and heat control. Thanks again.

Jeremy
Jeremy Lindley, Apprentice Smith
0

#5 User is offline   Russell Roosevelt 

  • Advanced Forum Member
  • PipPipPipPip
  • View gallery
  • Group: Members
  • Posts: 86
  • Joined: 18-July 10
  • LocationAlbion, IL.
  • ABS Rating:Journeyman Smith

Posted 26 September 2011 - 07:00 PM

Brian;

That was an excellent illustration!