Posted 27 May 2011 - 07:58 AM

Have any of you guys experienced more decarburization in 5160 over other steels?

Another question for you. Have you quenched 5160 and find the file cuts at first, then skates a little while later?

I dont think this is my imagination.
Lin Rhea, ABS Mastersmith
Email me
0

#2 User is offline   BrionTomberlin 

  • Administrator
  • Icon
  • View gallery
  • Group: Moderators
  • Posts: 608
  • Joined: 28-December 09
  • LocationNorman, Oklahoma
  • ABS Rating:Master Smith

Posted 27 May 2011 - 08:54 AM

No you are not imagining things Lin. I have found decarb on 5160 and 9260. Seems like more so on 9260. The first time I heat treated a piece of 9260 I thought I did something wrong because the file just dug right in. Went to the grinder and made some clean up passes and no more filing. Then of course I went duh! decarburization dummy.

It does seem to occur more on those two steels. I do not have a problem with 1084 or W-2.

I guess we should label this thread the Decarb Blues. You are not alone.
Brion
Brion Tomberlin
Anvil Top Custom Knives
ABS Mastersmith
0

#3 User is offline   Lin Rhea 

  • Advanced Forum Member
  • PipPipPipPip
  • View gallery
  • Group: Members
  • Posts: 449
  • Joined: 04-February 10
  • LocationPrattsville, Arkansas
  • ABS Rating:Master Smith

Posted 27 May 2011 - 10:59 AM

I just hardened two 9 inch blades and they are 5160. I had to take a couple thousandths of the edge and sides near the edge to reach the hard steel. It's not a problem, but sometimes I fail to remember and I get surprised all over again. :rolleyes:

I once hardened a blade 5 times before I figured it out. Doh!

Yep, 5160. That was back when I did dumb things.
Lin Rhea, ABS Mastersmith
Email me
0

#4 User is offline   BrionTomberlin 

  • Administrator
  • Icon
  • View gallery
  • Group: Moderators
  • Posts: 608
  • Joined: 28-December 09
  • LocationNorman, Oklahoma
  • ABS Rating:Master Smith

Posted 27 May 2011 - 07:39 PM

Got news for you Lin, I still do dumb things, :lol:. See you at the big show.
Brion
Brion Tomberlin
Anvil Top Custom Knives
ABS Mastersmith
0

#5 User is offline   Lin Rhea 

  • Advanced Forum Member
  • PipPipPipPip
  • View gallery
  • Group: Members
  • Posts: 449
  • Joined: 04-February 10
  • LocationPrattsville, Arkansas
  • ABS Rating:Master Smith

Posted 28 May 2011 - 11:11 AM

The blade is just right. I chopped boisdarc with it and it did well.

5160 has always been one of my favorites, but it goes to show you that you have to work it like it wants.
Lin Rhea, ABS Mastersmith
Email me